Stick Welding Tips, Certification tests, machines, projects
Post Reply
User avatar
  • Posts:
  • Joined:
    Wed Jan 28, 2015 7:27 pm
  • Location:
    Portugal

Received this box of rods from a sales agent for a tool mfg company. I had ordered regular 6013 rods though. So I thought they were 7018. Doesn't say on the box. Only has ISO number and I'm not familiar with that.

I welded a bit on a loader bucket today and the weld would crack right thru the middle after a while.
Attachments
20160117_090808.jpg
20160117_090808.jpg (29.58 KiB) Viewed 987 times
sedanman
  • Posts:
  • Joined:
    Sun Jan 03, 2016 2:54 pm
  • Location:
    Beacon and Pawling, New York

A google search and some translation from Italian suggests these are hardfacing rods. https://shop.berner.eu/it-it/p/132432-e ... _id=132432
User avatar
  • Posts:
  • Joined:
    Wed Jan 28, 2015 7:27 pm
  • Location:
    Portugal

Nice, just what I needed... :?
Artie F. Emm
  • Posts:
  • Joined:
    Thu Jul 24, 2014 7:53 am

The e6-um-60 comes up in a google search as a hardsurfacing electrode.
Dave
aka "RTFM"
Coldman
  • Posts:
  • Joined:
    Mon Dec 15, 2014 2:16 am
  • Location:
    Oz

They are hardfacing rods. DIN8555 calls up more than 0.5% carbon and significant manganese content plus other possible alloys like chromium. Which explains your cracking beads.
Flat out like a lizard drinkin'
User avatar
  • Posts:
  • Joined:
    Wed Jan 28, 2015 7:27 pm
  • Location:
    Portugal

For hard surfacing rods they actually weld good! I had no problem with fusion or laying a decent bead. And I cannot say that they were more difficult to grind flat either...

I have a box of real hard surfacing rods and i went to take a look at the. They only say Supradur 1000. No Din codes or other codes. They don't weld worth a :!: , almost have to long arc them. End up looking like bird crap... But when you want to grind them flat, sparks are deep dark red and you have a real hard time doing it!
gnuuser
  • Posts:
  • Joined:
    Sun Jan 31, 2016 12:10 pm
  • Location:
    USA

we use hard facing rods on the crusher at our glass plant and the welds look like a crackled mess afterwards but boy does it last a long time.
shooting the $#!t is a lot more fun when you use hollow points (more splatter);)