Tig welding tips, questions, equipment, applications, instructions, techniques, tig welding machines, troubleshooting tig welding process
User avatar
  • Posts:
  • Joined:
    Sun Sep 13, 2020 12:15 am
  • Location:
    Bay Area

Getting ready to take my first test for 2G, 1-1/2" OD x .095" 4130. so I have a few question and any advice is appreciated. First going to prep tube to 60 degree bevels. Is a root gap needed for this size tube? What size filler 1/16 or 3/32? Two passes?

Thanks, Kevin
"Be one with the weld"
Coldman
  • Posts:
  • Joined:
    Mon Dec 15, 2014 2:16 am
  • Location:
    Oz

Is there a Weld Procedure Specification for this test or maybe a code?
Flat out like a lizard drinkin'
Poland308
  • Posts:
  • Joined:
    Thu Sep 10, 2015 8:45 pm
  • Location:
    Iowa

60 deg seams like a lot of bevel, unless you mean both bevels together equaling 60. But it’s only .095 so not sure you can bevel that. Definitely won’t leave much room for land.
I have more questions than answers

Josh
User avatar
  • Posts:
  • Joined:
    Sun Sep 13, 2020 12:15 am
  • Location:
    Bay Area

Must meet D17.1 spec's. The bevels are 30 degrees, just not sure if needed for .095" of course has to be full pen.
"Be one with the weld"
Coldman
  • Posts:
  • Joined:
    Mon Dec 15, 2014 2:16 am
  • Location:
    Oz

I'd gap it 3/32" and with 3/32" wire, lay the wire flat and walk over it for the first pass at 80 amps to get motoring around fast. This prevents over penetrating and over heating. Let cool. Then I'd cap it with 1/16" wire 70 amps, this prevents over reinforcement.
Flat out like a lizard drinkin'
User avatar
  • Posts:
  • Joined:
    Sun Sep 13, 2020 12:15 am
  • Location:
    Bay Area

Thanks Coldman, I have material coming and I'll give it a try!
"Be one with the weld"
Post Reply